配方类型:
ELASTOMERS, POLYMERS, AND RESINS
配方说明:
Copolymer (Sodium Vinyl Sulfonate/Acrylamide)
配方组成:
Potassium Persulfate/0.050
Acrylamide/50.000
Sodium Bisulfite (0.1% aq. sol'n.)/0.025
Sodium Vinyl Sulfonate (25.0% aq. sol'n.)/50.000
Water/310.000
配制方法:
Charge water, acrylamide, and SVS to the reactor, start nitrogen purge, and heat to 50 C. At 50 C, add the potassium persulfate catalyst and allow to mix for a few min. Charge small amount of the bisulfite solution to initiate, and heat to 75-80 C. Maintain the temperature at 75-80 C for approximately 2 h. During the heating period, add the remainder of the bisulfite solution one drop at a time.
Total Solids---17.0% Brookfield Visc., 30 rpm---3900 cps