帮助中心
配方类型:
POLISHES
配方说明:
Wood Paneling Polish
配方组成:
Morpholine/1.0
Oleic Acid/2.0
"Tergitol" 15-S-12/2.0
Distilled Water or Equivalent/60.0
Mineral Spirits/20.0
"Union Carbide" L-45 (350 cSt)/5..0
"Carbopol" 941 (2% disp.)/10.0
配制方法:
Dissolve the "Tergitol" and morpholine in water in a vessel large enough to contain the final volume of polish. In a separate container dissolve the oleic acid and L-45 in mineral spirits. Slowly and the mineral spirits solution to the water solution with good agitation.
Slowly add the dispersion of "Carbopol" 941 resin with vigorous agitation and continue agitation as necessary to insure homogeneity of the formula.
Note: Above formulation is for a spray-can application. For a different package, a slightly higher level of "Carbopol" resin and morpholine may be required.
联系我们