Tung Oil/Linseed Oil, Vol/5/1 Mineral Spirits/368.0 Tung Oil/165.1 Lead Naphthenate, 24%/2.4 Cobalt Naphthenate, 6%/2.0 or 740.4 Bodied Linseed Oil, Z-6/33.8 "Panarez" 6-210 Hydrocarbon Resin/169.1 Non-Volatile Matter, wt%/50
配制方法:
Charge the kettle with all the resin and tung oil. Heat to 450'F in 45 minutes. Hold for body (approximately 2 hours and 30 minutes). Check with the linseed oil. Cool to 400'F and thin to 50% solids. Blend in the driers.