帮助中心
配方类型:
METALS
配方说明:
To Seal Porous Light Metal Castings (U.S. Patent 2,680,081)
配方组成:
Water/To make 100 cc
Chromic Acid/7 g
Potassium Dichromate/5 g
Waterglass/50 cc
配制方法:
The castings are placed in a vacuum and then in the solution at 95 to 100'C for half an hour at 60 to 80 lb/sq inch pressure.
联系我们