配方类型:
RUBBER, PLASTICS, WAXES
配方说明:
Polyester G
配方组成:
Phthalic Anhydride/22 g
Diethylene Glycol/584 g
Adipic Acid/219 g
Maleic Anhydride/686 g
Ethylene Glycol/341 g
配制方法:
Charge the glycols. Start the agitator and introduce a slow stream of inert gas. Heat to about 80'C and add the maleic anhydride, followed by the phthalic anhydride and the adipic acid. Raise the temperature to 150'C in 1 hour and then about 10'C per hour until the temperature has reached 210'C. Keep at 210'C until the acid number is less than 60.
Apply a vacuum of 100 to 200 mm and let the temperature fall to about 180'C. End the vacuum treatment when the acid number is below 40. Cool and add an inhibitor.