Octylene Oxide/10.0 The reactants are mixed and cured for 2 hr at 85'C and 4.5 hr at 150'C. This system is fluid at room temperature and has a pot life of about 24 hr at 25'C. 2) with Phthalic Anhydride Epoxy Resin (Epoxide equivalent 175-210)/100 Octylene Oxide/10 Phthalic Anhydride/75 Benzyl Dimethylamine/0.5 Diethylene Triamine/10.6 Epoxy Resin (Epoxide equivalent 175-210)/100.0 Epoxy Resin (Epoxide equivalent 175-210)/100 Methyl "nadic" Anhydride/85 Octylene Oxide/10 Benzyl Dimethyl Amine/2
配制方法:
The components are mixed and warmed to dissolve the phthalic anhydride. The curing cycle is 8 hr at 150'C.