帮助中心
配方类型:
POLISH
配方说明:
Emulsion of "Shanco" W-1119 Wax/Polyethylene
配方组成:
Morpholine/20
Polyethylene (Emulsifiable)/80
Water---(208-212'F)/610
Oleic Acid (Pale)/20
(Solids 16%)/750 lb
"Shanco" W-1119 Wax/20 lb
配制方法:
Heat the "Shanco" W-1119 Wax, polyethylene and oleic Acid to a fluid melt at 250'F. Add the morpholine and mix slowly for about 5 minutes.
Remove open flames before adding the morpholine. Adjust temperature of the base at around 240'F.
Have the water at 208-210'F, just under boiling and agitate rapidly to produce a vortex. Pour the hot base slowly into the side of the vortex at a rate that will not create boiling. Mix rapidly for 5 minutes. Cool while agitating slowly.