Xylene/8.20 Part Xylene/48.0 Soak Hypalon 20 chips 24 to 48 hours in Xylene and pony mix into Hypalon 20/22.6 solution. Catalyst for above quantity High Speed Mix or Roller Mill Grind Pebble Mill Magnesium Oxide (Light)/4.50 Staybelite Resin/0.57 Pigment, A or D-Series/29.4 "Tetrone" A/0.23
配制方法: