"Nytal" 300 Clay/60.00 Final pH-9.3 Viscosity, Brookfiled RVF, No.3 spindle, at 20 rpm-1,800 cP. Note: Increasing amount of plasticizer, Tricresyl phosphate, will increase flexibility in the foam. Total solids, 62.2% Pigment Grind Recip "Sipex" SB 8208/1.66 Ammonium Hydroxide/1.78 Tricresyl Phosphate/30.00 Ammonium Stearate/48.50 Pigment Grind/121.00 "Geon" 460X9/197.00 Water/44.20 "Good-Rite" K-718/8.00 Tetrasodium Pyrophosphate/0.50 Titanium Dioxide Slurry/25.70 "Monoplex" S-73/8.20 "Tamol" 850/1.50
配制方法:
Prepare the pigment grind with a Cowles blade attached to an air mixer. A Titanox RA-50 titanium dioxide slurry can be prepared by simply adding water. Mix the titanium dioxide slurry in a Lightnin' mixer, to 70% total solids.