1. Heat wax and fatty acid at 125-130'C (257-266'F) until molten. (a) Formulation No. 10: Predissolve KOH with warm ethylene glycol and add to melt at 125'C, (257'F) with agitation. Then stir until most of the foam disappears. 2. With continued agitation add amine and reheat to 125-130'C (257-266'F); (b) Formulation No. 11 only: Add ammonium hydroxide to heated water just prior to pouring molten mixture. (c) Formulations with agitation and reheat to 125-130'C (257-266'F) before pouring. 3. Pour with rapid agitation into water at 95-98'C (203-208'F); 4. Cool to room temperature with agitation. 5. For optimum emulsion quality, it is recommended that the molten wax mixture be introduced below the surface of water, close to the point of agitation during emulsification.