Cast a 6-mill wet film of the compound on a ferro-type panel at room temperature and dry at 66 C (150 F). In production the film could be applied by spraying. Lay the coated leather on top of the coated ferro-type panel. Press at 3.45 MPa (500 psi) and 93 C (200 F) for 30 s. Cool the laminate before removing it from the panel.