配方类型:
COATINGS
配方说明:
Water-Reducible Alkyd Baking Finish
配方组成:
Ammonium Hydroxide (28%)/31.2
Step 5:
Premix following first two components
Titanium Dioxide, R-900/307.20
Sol'n. made in Step 1/140.27
"Resimene" 745/61.44
Water/243.1
Sol'n. made in Step 1/140.27
"Chempol" 10-0500/564.0
Sol'n. made in Step 1/409.60/450.60
"FC"-430 (10% in water)/41.00/450.60
2-Ethylhexanol/10.24
"Byk"-H36/1.02
配制方法:
Mix well.
Add ingredients in order listed. Reduce to spray viscosity with 3 parts water for 5 parts enamel (by volume). Flash for 5-10 min and bake 15 min at 350'F.