prepare in a sigma blade mixer equipped with a jacket for steam and cold water using the following steps: start: steam on to 149 C (300 F); charge polybutene, antioxidant, stabilizer, calcium carbonate, silica, tio2. 5 min: add copolymer. 10 min: add resin 18. 30 min: add tackifying resin. 65 min: dump.