clean equipment with ethyl acetate to acetone. hardened cyanoacrylate can be removed by grinding or immersion in hot caustic. bonds can be separated by soaking in dimethylformamide or ethyl acetate or by heating to 200-250 C (400-500 F) hard clay/11.40 tall oil fatty acid/0.49 mineral spirits/3.33 "amoco" H-300 polybutene/-- cobalt drier (6%)/0.29 calcium carbonate/50.50 platelet talc/5.40 "keltrol"/4.39 "amoco" H-100 polybutene/21.00 diatomaceous silica/3.20
配制方法:
the vehicle ingredients blend in a dual arm sigma blade mixer. fillers are added incrementally in the order listed and then mixed 30 min. the mixture is thinned to desired viscosity with mineral spirits, the driers added, and the caulk mixed to a smooth consistency.