配方组成:
"ethomeen" C/25/0.25
"carbopol" 941/0.25
mineral oil/50.00
graphite//25.00
sodium hydroxide (10% sol'n.)/1.40
water/50.00
配制方法:
brookfield visc, 20 rpm-33,000 mPas or cP pH-10.2 carefully disperse the "carbopol" 941 resin in the water. after complete dispersion, add the sodium hydroxide and then the "ethomeen" C/25. disperse the graphite in the mineral oil. it is advisable to deaerate this mix before the next step because of the large amount of air absorbed ofn the graphite particles. thoroughly mix in the oil-graphite blend. stir to uniformity.
note: this formulation was designed to be diluted 3 to 1 with water and remain stable.