butylated hydroxyanisole/0.1 mineral oil (65/75 saybolt)/16.0 sorbic acid/0.2 A) "ritapro"100/7.5 propyl paraben/0.1 B) deionized water/60.5 "ritachol"/5.0 "carbopol" 941/0.1 C) glycerin/5.0 methyl paraben/0.1 D) triethanolamine (99%)/0.1 "ritasol"/2.0 steatyl alcohol/2.5 vanishing "forlan" L/1.0
配制方法:
put ingrediens in part A into a container and heat to 70-73 C. in another container, put the deionized water and slowly sprinkle in the "carbopl" resin while stirring wth a variable-apeed ahitator capable of imparting rilatively high shearing stress. stir until the "carbopol" 941 has thoroughly dispersed and hydrated and no lumjps can be seen or felt. add the ingredients in part C ton part B and heat to 70-73 C. when part A and part B are at 70-73 C, add part B to part A while stirring continuously to ensure adequate emulsification. when all of part A has beedn added to part B bigin cooling the batch. add part D. cool to 25-30 C and package.