heat resin 18 in solvent at 80 C until dissolved. add preheated (80 C) polybuene and stir. pour solution over TPE and heat 15 min in overat 99 C. place on pebble mill for 2-3 h. altetrnately heat and roll until homogeneous.heat to 80 C and mix in high-speed stirrer at 2000 rpm. gradually add preheated (80 C) emulsifiers and antioxidant. add boiling water slowy until inuersion occurs. add remaining water. mix for 10 min. blend in tackifier and latex.