帮助中心
配方类型:
EMULSIONS AND OTHER COLLOIDS
配方说明:
"Armowax" Emulsion
配方组成:
Glacial Acetic Acid/0.6
"Armowax"/20.0
Water/76.0
"Ethomeen" 18/12/3.4
配制方法:
Heat the "Armowax" and "Ethomeen" to approximately 140'C. (284'F.).
Add this mixture in a thin stream to the water and acetic acid heated to approximately 100'C. (212'F.), using vigorous agitation. continue stirring until smooth. for maximum fineness of particle size, use a colloid mill or equivalent.
Lumping in the initial stage is a natural occurrence and will thin out on continued agitation.
联系我们
咨询反馈