4% Calcium naphthenate/6 lb. "Amsco" 140L (to satisfactory viscosity)/33 lb. Dipentene/24 lb. Mix A 15 minutes. Mix B 5 minutes. Mill: Use 80 Stator, 46 Rotor. One pass through Morehouse Mill. Set stones 2/1000 off positive tight, at a cold start. Reset 4-5/1000 off positive tight, after maximum warm up of mill. Let Down "RCHTX"/100 lb. "Thixcin"/3 lb. A: "Amsco" 140L/100 lb. "Ti-pure" R-110/200 lb. "D-65A"/300 lb. B: "D-65A"/48 lb. "Castung" 103 G-H/40 lb. "Dustex" Micro-Silica/100 lb. 24% Lead Naphthenate/4 lb. "D-65A"/90 lb. 6% Cobalt Naphthenate/2 lb. "Dipentene"/7 lb.
配制方法:
Production Rate: 8-12 gal. per hour -Model -M Over 100 gal. per hour -Model -B1400 Grind: 6-7 N.S. When 80 over 46 suggested stones are employed they should be sealed (used) stones. To get the same results with new stones use 80 over 60 grit.