4% Calcium Naphthenate/3 lb. "Amsco" 140L (to satisfactory viscosity)/40 lb. Mix A 15 minutes. Mix B 5 minutes. Mill: Use 80 Stator, 46 Rotor. One pass through Morehouse Mill. Set stones 2/1000 off positive tight, at a cold start. Reset 4-5/1000 off positive tight, after maximum warm up of mill. Let Down "RCHTXX"/250 lb. "D-65A"/137 lb. A: "Amsco" 140L/100 lb. "Ti-pure" R-110/100 lb. "D-65A"/260 lb. B: "D-65A"/13 lb. "Castung" 102 G-H/24 lb. "Dustex" Micro-Silica/200 lb. 24% Lead Naphthenate/6 lb. "Thixcin"/3.5 lb. 6% Cobalt Naphthenate/2 lb. Dipentene/21 lb.
配制方法:
Production Rate: 8-12 gal. per hour -Model -M Over 100 gal. per hour -Model B-1400 Grind: 4-5 N.S. Temperature can be controlled to range of 110 to 150'F. by stone clearance. Appearance (24 hours) very good in all respects. When 80 over 46 suggested stones are employed they should be sealed (used) stones. To get same results with new stones use 80 over 60 grit.