配方类型:
METALS AND THEIR TREATMENT
配方说明:
Refractory Mixture
配方组成:
Sand (140 Mesh)/45.0
Magnesium Oxide/0.4
Sand (35-60 Mesh)/20.0
Silica Flour/34.6
配制方法:
To insure even distribution of the magnesium oxide, mix it with the silica flour and then add this mixture to the sand. Magnesium oxide is incorporated as a neutralizing agent for the hydrochloric acid.
Satisfactory results are obtained by mixing 100 cc. (3.4 oz.) of the binder solution with 1 lb. of the refractory mixture. This blend is poured around the wax pattern, settled on a vibrating table, and allowed to gel.
Where a smooth casting and reproduction of fine detail are necessary, a fine-grained refractory composition should be in contact with the fusible pattern. This can be accomplished most economically by using a primary dip coat followed by backing up with the regular investment.