Prepare a 2% stock solution of Ucare Polymer JR 400 by dispersing 2.0 parts of Ucare Polymer JR 400 in 98 parts of mildly agitated water at 20-25 C. When the polymer is completely wetted, heat to 60-70 C and agitate for approximately one hour until the solubilization is complete. Allow to cool with stirring. Mix together while stirring the Ucare Polymer JR 400 solution, Mirataine CBS, and Miranol C2M Conc. N.P. Add the water, Maprofix ES, Cedepal TD 404M, and Cerasynt IP. Heat and mix until uniform making sure that the Cerasynt IP has dissolved. Cool with stirring. Adjust the pH to 6.7 with hydrochloric acid. Physical Properties: Solids---15.7% Visc.---4000 cps