帮助中心
配方类型:
MISCELLANEOUS
配方说明:
Screen Printing Dye Concentrate
配方组成:
"Tween" 80/6.0
"Carbopol" 846/7.5
"Sipex" SB 29%/8.6
"Kaydol" Mineral Oil/-
Recommended Application/Screen or roller
"Carbopol" 820/7.5
Water/30.4
"Span" 80/5.0
"Isopar" M/28.0
Ammonium Hydroxide (28%)/7.0
配制方法:
Add the "Carbopol" resin(s) to the blend of oil, hydrophobic surfactant, and antifoam. Agitate slowly for 5-10 min. Premix the ammonium hydroxide and water. Slowly add the dilute ammonium hydroxide solution to the wetted-out mixture of "Carbopol" resin. For best results, add the solution at a constant rate. If a variable drive mixer is available, increase the agitation from slow to moderate or higher.
Mix for 15-20 min after all the ammonium hydroxide has been added. Add the hydrophilic surfactant and mix for 5-10 min.
联系我们