帮助中心
配方类型:
MISCELLANEOUS
配方说明:
Graphite-Mineral Oil Mold Release
配方组成:
pH/10.2
"Ethomeen" C/25/0.25
"Carbopol" 941/0.25
Mineral Oil/50.00
Graphite/25.00
Sodium Hydroxide (10% sol'n.)/1.40
Water/50.00
Brookfield Visc., 20 rpm---33,000 mPa.s or cP
配制方法:
Carefully disperse the "Carbopol" 941 resin in the water. After complete dispersion, add the sodium hydroxide and then the "Ethomeen" C/25. Disperse the graphite in the mineral oil. It is advisable to deaerate this mix before the next step because of the large amount of air absorbed on the graphite particles. Thoroughly mix in the oil-graphite blend. Stir to uniformity.
Note: This formulation was designed to be diluted 3 to 1 with water and remain stable.