Mineral Spirits/7.8 Barytes/13.0 Hydrogenated Castor Oil/1.0 Chlorinated Rubber, 20 cps./16.2 Soya Oil, epoxidized/1.0 Metallic Lead paste, 91% in Oil/30.0 Aromatic naphtha (320-350'F)/24.0 Chlorinated Paraffin/7.0
配制方法:
Grind barytes in plasticizer. Add hydrogenerated Castor Oil, warm the mixture and stir in to assure good dispersion. Then add chlorinated rubber solution and finally the lead paste.