配方类型:
TEXTILE SPECIALTIES
配方说明:
Nonwoven Fabric Binder
配方组成:
Water/30.0 lb
The webs are usually sprayed on both sides either as they emerge from
the crosslapper or by spraying one side, running the web through the
oven and spraying the other side after the web turns over a roll for the
return trip through the oven. A combined dry and cure time of 3 min at
325'F is desirable, but but both lower and higher temperatures have been
found satisfactory with some time adjustment.
Saturation Bonding
No.
"Dow Corning" Antifoam A^2/500.0 cc
"Triton" X-100/50.0 g
Ammonium chloride or/50.0 g
"Poly-Tex" Emulsion (46% NV)/20.0 lb
"Poly-Tex" Emulsion (46% NV)/72.0 lb
Water/144.0 lb
Oxalic acid/40.0 g
Ammonium chloride or oxalic acid/4.5 oz
"Triton" X-100/4.5 oz
配制方法:
The drying and curing requirements will be generally the same as used for the spray-bonded web. In either case where a nonreactive emulsion is used, the catalyst may be omitted or where a cellulosic fiber is involed, the use of a small amount (5-15%) of a catalyzed urea or melamine resin such as Aerotex M-3 may prove desirable.
As might be expected, spray bonding is normally used for the loftier webs, commonly called fiber fill, and saturation bonding is used for denser webs such as apparel interliners, sheets, gowns, etc.