配方类型:
POLISH
配方说明:
Semibuffable Floor Finish
配方组成:
"UBS" polymer WC-30 at 14% solids/62.5
"DURON" 180D/
"KP"-140/1.0
"DURON" 195D/
"AC"-680/
Oleic acid/4.0 g
Ammoniacal solution of "Durez" 19788/12.5
KOH at 45%/3.0 g
Morpholine/11.0 g
1% Aqueous solution of FC-128/1.0
Wax base No. 7165*/25.0
Water at 205'F/
Water at room temperature/400.0 g
*Wax---Polyethylene emulsion Base No. 7165
Methyl "Carbitol"/2.0
"RUHRWAX" AV-1551/25.0 g
配制方法:
melt the waxes, the "AC"-680 and the oleic acid together, add KOH solution at approx. 230'F and react for 20 to 30 min with mild agitation, until the batch clears and foaming ceases. Increase the temperature to 250'F and add the Morpholine. Stir until clear.
Maintaining the wax melt at 250 to 255'F, pour it slowly with rapid agitation into the 232 g of water at 205'F. Continue agitation and heating for an additional 1 to 2 min after all the wax has been poured.
Cool rapidly to rom temperature with mild agitation, and then add the emulsion th toe rest of the water at room temperature.