Wax-polyethylene base 6866*/25.0 "Durmont" E/40.0 "Carbitol"/1.0 "Epolene" E-15/5.0 "Acintol" FA3/3.0 KOH at 43%/3.0 Ammoniacal solution of "Durez" 19788/7.5 3-Methoxy propylamine/15.0 Ammonia 28%/226.0 FC-128 at 1%/0.5 "Rhoplex" B336/67.5 Water at 195'F/402.0 Water at room temperature *Wax-Polyethylene base/30.0 "KP"-140 or equiv. TBEP/1.0 "Duron" 180-D/30.0
配制方法:
Melt the waxes, "Epolene" and fatty acid together, add KOH solution at 225'F, and react without stirring 20 to 30 min until batch clears and foaming ceases. Add the 3-MPA. Readjust melt to 255'F. Bring water temperature (226 g portion) to maximum 200'F. Start highspeed agitation and add the NH3OH to the water. Slowly pour melt into the ammoniated water with consistent agitation. Hold at heat for 1 to 2 min, then add balance of watr. Cool to room temperature and store or use in polymer blend.