配方类型:
POLISH
配方说明:
Rubless Floor Polish
配方组成:
"EPolene" E-12/20.0
Melt the "Durmont", "Duron", polyethylene and oleic acid together,
and cook with the KOH at about 240'F for 20-30 min, until the batch
becomes clear and foaming has ceased. Then add the morpholine. Stir
until clear. Adjust the melt temperature to 240 to 245'F. Pour the melt
into water of 203 to 205'F with strong agitation. Avoid foaming and
surface boiling, as these may cause graininess and to loss foaming and
surface boiling, as these may cause graininess and loss of film clarity
and gloss. Continue heat and agitation for 1 to 2 min after all the wax
has been dispersed. Then turn on the cooling watr and agitate slowly
until the batch reaches room temperature.
Formula No.7
This formula yields a product of exceptionally white, translucent
appearance which is nondiscoloring because it makes use of a water-clear
leveling resin and an emulsifier system which, in contrast to morpholine
oleate, does not stain certain sen
配制方法:
Add with light stirring in the order as shown. To incorporate the plasticizer system, use high speed agitation for 30 min.
Melt "Efton", "Durmont", "Epolene", oleic acid and "Tween" 80 together, raise the temperature to 240'F and react without stirring with the KOH solution for 20 to 30 min until the batch clears and foaming ceases.
Then add the mixture of 3-methoxy propylamine and aminomethyl-propanol.
Stir until clear. Pour the melt at 240 to 245'F into water at 203 to 205'F with strong agitation. Avoid foaming or surface boiling.
Temperatures are important! Continue heat and agitation about 2 min after all the wax has been dispersed. Then turn on the cooling water and agitate slowly to room temperature. Cover the batch to avoid skin formation.