配方类型:
METALS AND THEIR TREATMENT
配方说明:
Coloring Copper Blue
配方组成:
Gelatin/0.5 oz/gal
Cathode current density/1.5 to 4 A/ft^2
Copper acetate/1.5 oz/gal
Formula No.
Sodium thiosulfate/8 oz/gal
Lead acetate/4 oz/gal
Temperature/200'F
Immersion time/30 to 60 sec.
配制方法:
At temperatures below about 170'F, thin yellow, green, or red films are obtained, depending on the immersion time. With an addition of potassium.