"DW"-855 (15%)/70.0 Diethylene glycol monoethyl ether/2.0 "AC"-680 (15%)/10.0 Ethylene glycol/1.0 "Shanco" 6000 Resin (15%)/20.0 Blend the "Shanco" 6000 Resin solution into the polymer emulsion, then add the "AC"-680 emulsion. Premix the plasticizers and surfactant and blend into the previous mixture. Agitate for thirty minutes, then adjust the final pH to 8.5 to 9.0 with 28% ammonia "AC"-680/80.0 Oleic acid/14.0 "FC"-128 (1%)/0.4 Morpholine/14.0 Tributoxyethyl phosphate/1.0 Water (208-210'F)/518.7
配制方法:
Bring "AC"-680 and oleic acid to fluid melt at 230-240'F. Blend well, add morpholine, and mix for five minutes. Slowly pour melt into t he agitator vortex of the hot water and mix for five minutes at 208-210'F, then cool rapidly to room temperature with continuous mixing.