Heat the paraffin wax, "Ethofat," and "Ethomeen" to 150'F. until liquefied. Add 10 parts of water (heated to 150'F. or over) slowly with paddle agitation to disperse the emulsifier thoroughly. Add the balance of hot water rapidly, using the same type of agitation. Agitate until the emulsion comes to 140'F. Hold and add the acetic acid, using the same agitation. Continue agitating until 120'F. is reached. Add the "Lomar" P.W. and continue the agitation until cooled to room temperature. cool slowly.