配方类型:
COATINGS
配方说明:
Polyester Coating for Wood
配方组成:
Styrene (monomer)/47.25
Methyl ethyl ketone peroxide/1.00
Half-Second Butyrate/4.00
Viscosity, 77'F., cp./180.00
X5841-25 (solid resin)*/47.25
Lb./gal/8.92
Cobalt naphthenate (6% metal)/0.50
配制方法:
The solid resin is heated to 250'F and the Half-Second Butyrate then added with agitation, followed by addition of the styrene. this solution is very stable at room temperature as the inclusion of Half-second Butyrate does not affect its stability. the two catalysts, cobalt naphthenate and methyl ethyl ketone peroxide, are added to the solution immediately before application of the coating.